   IndiaRubberDirectory.com > Rubber Engineering > Standard Rubber Formulations

Standard Rubber Formulations - CARPET BACKING

CARPET BACKING

    Parts by wt.

60% NR latex                         

167

20% KOH solution

1.5

20% Lissapol D solution *  

20.0

Dispersol VL (20% solution) 

5.0

50% Sulphur dispersion

3.0

50% Accicure ZDC dispersion

2.0

40% Zinc oxide dispersion    

7.5

20% SP emulsion     

2.0
China clay (added as a 50%  slurry)         200.0
Pigment dispersion              as required

Cure in hot air at 110°-120°C : 15 minutes 

*Half is added to china clay slurry before addition to the compound.

  Rubber Engineering

Rubber Product Manufacturers

Get listed in IRD
Premium listing in IRD

 

 

 

 



 

 










New Page 1

    Rubber Articles
   Technical Papers
   Press Releases
   Rubber Articles
   Rubber Statistics
 
 
 
 
 
 
 
 




Contact Us : www.indiarubberdirectory.com C/o Team Web Power, No.52, First Floor, Anna Nagar Plaza, C-47, IInd Avenue,
Anna Nagar, Chennai 600040. India. 
Phone:- +91-44-42170137 Mobile:- +91-9444001705

|    About Us    |    Vision    |    Disclaimer    |    Privacy Policy     | Sitemap     |    Feedback    |    Contact Us    |    Home    |

Contact Us : www.indiarubberdirectory.com , No.52, First Floor, Anna Nagar Plaza, C-47, IInd Avenue, Anna Nagar, Chennai 600040.Tamilnadu, India.

Phone: +91-44-42170137  Mobile: +91-9444001705  Email:
rubberdirectory@gmail.com